Abstract
The luminous efficiency of white light-emitting diodes, which are used as light sources for next-generation illumination, is continuously improving. Presently available white light-emitting diodes emit with extremely high luminance because their emission areas are much smaller than those of conventional light sources. Consequently, white light-emitting diodes produce a glare that is uncomfortable to the human eye. Here we report a yellow-emitting phosphor, the Eu2+-doped chlorometasilicate (Ca1-x-y,Srx,Euy)7(SiO3)6Cl2, which can be used to create glareless white light-emitting diodes. The (Ca1-x-y,Srx,Euy)7(SiO3)6Cl2 exhibits a large Stokes shift, efficiently converting violet excitation light to yellow luminescence, and phosphors based on this host material have much less blue absorption than other phosphors. We used crystal structure analysis to determine the origin of the desired luminescence, and we used (Ca1-x-y,Srx,Euy)7(SiO3)6Cl2 and a blue-emitting phosphor in combination with a violet chip to fabricate glareless white light-emitting diodes that have large emission areas and are suitable for general illumination.
Similar content being viewed by others
Introduction
Recently, white light-emitting diodes (LEDs) have been receiving attention as light sources because of their energy efficiency1,2. The major white LEDs presently in the market are phosphor-converted LEDs (pc-LEDs) made of a blue InGaN chip and a yellow phosphor, (Y,Gd)3(Al,Ga)5O12:Ce3+ (abbreviated YAG:Ce3+)3. Its luminescence efficiency exceeds that of fluorescent lamps4,5. However, as pc-LEDs have much smaller emission areas than conventional light sources, their luminance rises excessively with increasing luminous efficiency, and consequently they produce an uncomfortable glare6. The emission areas of pc-LEDs are small, because the yellow-emitting phosphor must be located close to the blue chip to produce a uniform hue; therefore, the phosphor layer is typically deposited on the blue chip so that the chip and the layer have the same geometric area.
There have been many reports describing the development of phosphors7,8,9,10,11,12,13,14,15,16 for violet chips, which have an external quantum efficiency that is intrinsically higher than that of blue chips17,18,19. A pc-LED with a violet chip generates white light only from the luminescence of the phosphors. However, none of the previous reports dealt with glare suppression, which is a major obstacle to the practical application of pc-LEDs. In a pc-LED with a violet chip, two or more phosphors must be mounted on the chip. A combination of blue and yellow phosphors, or a combination of blue, green and red phosphors, is commonly used in pc-LEDs. Glare can be suppressed by expanding the emission area, but such expansion leads to a non-uniform hue. As the green, yellow and red phosphors emit undesirable luminescence by absorbing the light emitted from the blue phosphor20, therefore, phosphors that are not excited by the blue light are required. We approached this problem by tuning the excitation properties of the phosphor.
In this article, we report a new phosphor, (Ca1-x-y,Srx,Euy)7(SiO3)6Cl2 (abbreviated Cl_MS:Eu2+), which emits yellow luminescence upon violet excitation, with an internal quantum efficiency (IQE) higher than 90% and very weak absorption in the blue wavelength region. These properties allowed us to fabricate a pc-LED composed of a violet chip combined with Cl_MS:Eu2+ and a blue phosphor, (Ca,Sr)5(PO4)3Cl:Eu2+ (APT:Eu2+)21. This pc-LED had luminous flux, colour temperature and colour-rendering index values that were adequate for practical use, and it emitted white light with a uniform hue and suppressed glare, thus satisfying the requirements for general illumination. The host, Cl_MS, is a new material with a unique layered structure discovered in this work.
Results
Search for a phosphor material
In our search for an appropriate phosphor, we explored chemically stable oxide-based materials activated with Eu2+, which allows 5d–4f transitions. We considered the following features when designing the host material. The primary feature was a mixed-ligand system. In most Eu2+ oxides, Eu2+ absorbs in the ultraviolet wavelength region. Shifting the absorption band to the violet region requires a relatively large crystal-field splitting. A strong crystal field is generated when Eu2+ is located at a site with a distorted co-ordination field22, and such a site can be created with a mixed-ligand system. Here we chose oxide and chloride ions as the ligands. The second feature was a layered structure. To obtain a chemically stable phosphor, we chose a host with a layered structure of hydrophilic metal chloride layers alternating with oxide layers. We expected the layering to stabilize the chemically unstable metal chloride layer. As phosphors with layered structures often suffer from substantial thermal quenching of luminescence owing to loose interlayer bonding23,24, we explored materials that exhibited a small degree of thermal quenching.
A survey of materials conducted with these features in mind led us to focus on chlorosilicates25,26,27 and ultimately to design a new phosphor material, Cl_MS:Eu2+.
Crystal structures of Cl_MS and Cl_MS:Eu2+
We determined the crystal structures of an undoped Cl_MS single crystal and several Eu2+-doped powder samples by using synchrotron radiation X-ray diffraction (SR-XRD) at the SPring-8 synchrotron facility in Japan (see Supplementary Methods and Supplementary Tables S1 and S2). The structure of Cl_MS:Eu2+ was found to consist of alternating metal silicate and metal chloride layers along the c axis of a monoclinic unit cell (Fig. 1a). The chemical composition of Cl_MS:Eu2+ was determined to be (Ca1-x-y,Srx,Euy)7(SiO3)6Cl2 (0.167 < x/(1–x–y) < 2.5; 0.01 < y < 0.3). Cl_MS:Eu2+ had three cationic sites referred to as M(1), M(2) and M(3), which could accommodate Ca, Sr or Eu. The M(1) site in the metal silicate layer was occupied only by Ca and was co-ordinated by six oxide ions of Si3O9 units28 to form a [Ca(SiO3)6] framework (see Supplementary Fig. S1). The M(2) site was in the metal chloride layer and was occupied by a Sr or Eu ion. This site was co-ordinated by a chloride ion in the metal chloride layer and by seven oxide ions, and thus the site bridged the two metal silicate layers (Fig. 1b). The M(3) site at the boundary between the metal silicate and metal chloride layers was occupied by a Ca, Sr or Eu ion, and was co-ordinated by five oxygen ions in the metal silicate layer and by two chloride ions in the metal chloride layer (Fig. 1b). We have provided crystal information files in the Supplementary Data Sets 1 and 2. Supplementary Data Set 1 includes the crystal structures of an undoped single crystal of Cl_MS at 100 and 300 K. Supplementary Data Set 2 includes the crystal structures of Cl_MS:Eu2+ at 100 and 300 K.
Luminescence spectrum of Cl_MS:Eu2+
The luminescence spectrum of (Ca0.37Sr0.53Eu0.10)7(SiO3)6Cl2 obtained with a 400-nm excitation at room temperature exhibited a single band at 580 nm, with a full width at half-maximum of 3.6×103 cm−1 (Fig. 2a). The corresponding excitation spectrum exhibited strong absorption at wavelengths of 410 nm or shorter, but the intensity of the absorption rapidly decreased at wavelengths longer than 420 nm. Consequently, an ~450-nm blue light was only weakly absorbed by Cl_MS:Eu2+. Thus, the excitation spectrum of Cl_MS:Eu2+ distinctly differed from the excitation spectra of other phosphors used for violet excitation. For example, the excitation spectra of (Ba,Sr)2SiO4:Eu2+ (ref. 29) and (Sr,Ca)AlSiN3:Eu2+ (refs 30,31) exhibit considerable absorption intensity around 450 nm (Fig. 2a). In addition, the magnitude of the Stokes shift (ΔS) for Cl_MS:Eu2+ was 6.9×103 cm−1, which was much larger than that observed for conventional phosphors (Fig. 2a). The emission colour of Cl_MS:Eu2+ could be tuned by varying the Ca/Sr atomic ratio. We examined the Ca fraction dependence of the dominant wavelength (that is, the wavelength of monochromatic light that was the same colour as the band luminescence), and found that as the Ca/Sr ratio was increased the dominant wavelength was linearly red-shifted (Fig. 2b). The IQEs and absorptions at the dominant wavelength were almost equivalent. The luminescence spectra of typical samples are shown in Supplementary Fig. S2. The luminescence intensity of Cl_MS:Eu2+ was stable to Eu2+ concentration and temperature. Even though the Eu2+ concentration in Cl_MS:Eu2+ increased by more than 20 atom%, the samples consisted almost completely of a single phase that contained only a few impurities (see Supplementary Fig. S3). No concentration quenching occurred at Eu2+ concentrations up to 20 atom% (Fig. 2c and Supplementary Table S3). The highest luminescence intensity was observed at a dopant level of 10 atom%, (Ca0.37Sr0.53Eu0.10)7(SiO3)6Cl2, and the IQE and the absorption were 94% and 90%, respectively, upon excitation by a 407-nm laser diode. A luminescence intensity of 75% relative to the room temperature value was observed at 423 K (Fig. 2d). This temperature dependence was comparable to that of YAG:Ce3+. A life test in air at 85% humidity and 358 K showed that the variation in luminescence intensity was within 2% after 2,000 h; this variation was less than the variation observed for (Ba,Sr)2SiO4:Eu2+ after only 500 h of testing (Fig. 2e).
Eu2+ sites of Cl_MS:Eu2+
Upon excitation with ultraviolet radiation (Fig. 3a), a peak at 480 nm appeared in the luminescence spectrum of (Ca0.40Sr0.56Eu0.04)7(SiO3)6Cl2. The excitation spectrum of this emission band (480 nm) differed from that monitored at 580 nm; the former spectrum exhibited a narrow band peaking at 310 nm with weak violet absorption. This result confirmed that Cl_MS:Eu2+ had two different Eu2+-occupied sites, the M(2) and M(3) sites (Fig. 1b). To clarify the correspondence between the two crystallographic sites and the emission bands, we investigated the temperature dependence of the luminescence intensity and of the crystal structure. We plotted the radiative decay curves for (Ca0.40Sr0.56Eu0.04)7(SiO3)6Cl2 at 100 and 300 K upon excitation with a 266-nm laser pulse with monitoring at 480 and 580 nm (Fig. 3b,c). All the decay curves consisted of fast and slow components (with lifetimes τ1 and τ2, respectively), and were fitted by double exponential components. Here we discuss the fast component of each decay curve. The shorter lifetime of the 480-nm band (τ1) showed large temperature dependence between 100 and 300 K, whereas neither τ1 nor τ2 of the 580-nm band changed substantially with temperature. The SR-XRD analysis (Fig. 3d) revealed that the local structure of the M(2) site changed markedly with increasing temperature; three of the seven M(2)–O bonds lengthened by more than 0.02 Å. In contrast, the bond lengths at the M(3) site did not change markedly with increasing temperature (Fig. 3d). Consequently, we attributed the 580-nm band to Eu2+ at the M(3) site and the 480-nm band to Eu2+ at the M(2) site.
Discussion
The M(3)-site Eu2+ ion, which gave rise to the 580-nm band, was co-ordinated by the mixed ligand, that is, a single bridging oxygen ion, four non-bridging oxygen ions and two chloride ions (Fig. 1b), and was located at the boundary between the metal silicate and metal chloride layers. The asymmetric coordination structure of the M(3) site resulted in a large crystal-field splitting and an absorption band at a wavelength in the violet region, but not extending to the blue region. We evaluated the asymmetry of the Eu2+ sites by calculating electrical field gradients (EFGs) for the M(2) and M(3) sites using density functional theory (DFT). The initial structural parameters were taken from single-crystal SR-XRD data for CaSr2(Ca0.55Sr0.45)4Si6O18Cl2 at 100 K. In the calculation, we modelled the mixed occupation of the M(3) sites with Ca and Sr by the ordered structure shown in Supplementary Fig. S4. To obtain a relaxed structure, we optimized the geometry with the Vienna Ab Initio Simulation Package code32 using the projected, augmented plane-wave method33. The EFG parameters were calculated with the WIEN2k programme package34, which adopts a full-potential, all-electron method that utilizes the full-potential, linearized, augmented plane-wave+local orbitals approach35. In each calculation procedure, the exchange and correlation potentials within the DFT were calculated with the Perdew–Burke–Ernzerhof generalized gradient approximation36. The principal axes of the EFG tensors of the Sr2+ and Ca2+ ions at the M(2) and M(3) sites, respectively, are illustrated schematically in Fig. 4a, and the EFG tensor elements at the M(2) and M(3) sites calculated by DFT are summarized in Table 1. The asymmetry parameters η of the M(2) and M(3) sites could be derived by using the EFG tensor elements (defined at the bottom of Table 1). The value of η at the M(3) site was clearly much higher than that at the M(2) site.
The changes in the local structure of the M(3) site due to the increase in the Ca fraction induced a red shift of the luminescence. Anisotropic lattice contraction occurred along the a axis (see Supplementary Fig. S5), owing to shortening of the O(5)–M(3)–O(6) bonds with increasing Ca fraction (Fig. 4b). This contraction induced substantial deformation around the M(3) site. As such deformation widened the crystal-field splitting, the 580-nm luminescence band was red-shifted by a reduction of the lowest 5d energy level. These results are consistent with the calculated results, indicating that the η value for Ca at the M(3) site was larger than that for Sr (Table 1).
Cl_MS:Eu2+ exhibited a high IQE. IQE is given by Yamamoto37
where W is the luminescence radiation probability and N is the non-radiative transition probability. The main factors that affect the non-radiative transition probability are thermal quenching and concentration quenching. The IQE of Cl_MS:Eu2+ was very high because the influence of these factors was small owing to the following reasons.
Thermal expansion of Cl_MS:Eu2+ was anisotropic. The lattice constants increased linearly with increasing temperature from 100 to 573 K as shown in Supplementary Fig. S6. The linear thermal expansion co-efficient along the c axis, the direction perpendicular to the layers, was larger than that along the a- and b axes. The values along the c-, a- and b axes at 300 K were 1.8×105, 5.4×106 and 7.5×106 K−1, respectively. At the M(2) site, which bridged the metal silicate layers, the cation–oxygen bond lengths were markedly increased by thermal expansion of the interlayer separation. These lengthened bonds resulted in a shorter luminescence lifetime for the 480-nm band. In contrast, the change in the Eu2+–anion distance was less at the M(3) site, which had few co-ordinated oxide ions in the stacked-layer direction. Consequently, thermal quenching of the 580-nm band was sufficiently small for practical applications, despite the material's layered structure.
Concentration quenching of the main emission band (the 580-nm band) of Cl_MS:Eu2+ was not observed (Fig. 2c), but the 480-nm band was drastically affected by concentration quenching (see Supplementary Fig. S7). We cannot explain, on the basis of the experimental results, why concentration quenching of the M(3) site did not occur. The conspicuous difference in the sensitivity of the M(2) and M(3) sites to concentration quenching appears to have to do with local asymmetry around each site, which controlled the energy transfer processes from the excited Eu2+. There have been reports indicating that phosphors with a low-dimensional arrangement of the dopant ions show little concentration quenching38. In such phosphors, the stoichiometric phosphors (100% dopant ion) are also contained39,40. The dopant ion site of these phosphors has higher asymmetry, owing to low-dimensional arrangement. This observation is consistent with the fact that the M(3) site, which had lower symmetry and a low-dimensional arrangement, did not exhibit concentration quenching.
To evaluate the practical applicability of the Cl_MS:Eu2+ phosphor, we fabricated three sample pc-LEDs consisting of a violet or blue chip encapsulated in translucent resin containing various phosphors (Fig. 5a). Sample 1 was prepared with a violet chip coupled with (Ca0.37Sr0.53Eu0.10)7(SiO3)6Cl2 and the blue phosphor APT:Eu2+ (Fig. 5b). For reference, we also prepared pc-LEDs of the same structure with a blue chip coupled with YAG:Ce3+ (sample 2, Fig. 5c) and with a violet chip coupled with three primary-colour phosphors (sample 3, Fig. 5d). The differences in the emission colour distribution in the emission area of these three samples were measured with a two-dimensional colour analyser (Fig. 5e,f,g). Sample 1 exhibited a uniform hue over the entire resin dome, similar to that of an incandescent lamp, but samples 2 and 3 showed red-shifted colour on the rim of the dome, resulting in a non-uniform hue. The performance of these three samples is summarized in Supplementary Table S4.
Sample 1 exhibited a luminous flux of 88 lm and a luminance of 1.0 cd mm−2 at an operating current of 350 mA. For comparison, a surface-mount device (SMD) pc-LED, which is a commonly used type of pc-LED, exhibited a luminous flux of 85 lm and a luminance of 11 cd mm−2. The SMD pc-LED consisted of a thin phosphor layer deposited on a chip mounted at the bottom of a small casing (see Supplementary Fig. S8). The unified glare rating (UGR), which is used to evaluate glare, is given by the CIE41
where Lb is the background luminance (cd m−2), L is the source luminance (cd m−2), ω is the solid angle of the source (sr) and p is the position index (the positional relationship between the light source and the line of sight). The form of this equation indicates that as the source luminance increases, UGR rises and glare becomes uncomfortable. In sample 1, the luminance was reduced to less than 1/10 of that for the SMD pc-LED without a decrease in luminous flux; thus, unwanted glare was suppressed (see Supplementary Methods and Supplementary Fig. S9).
After continuous operation at 350 mA for 3,000 h, the luminous flux of sample 1 was still at least 96% of its initial value. The colour temperature was 4,100 K for sample 1, and the temperature could be tuned from 3,010 to 5,070 K by varying the Ca fraction (Fig. 5h).
We also fabricated a line-shaped module consisting of a row of pc-LEDs fabricated with Cl_MS:Eu2+ (Fig 5i,j). The module contained 18 violet chips aligned with a pitch of 8 mm. The chips were encapsulated thickly in a semi-cylindrical form, with resin containing Cl_MS:Eu2+ phosphors. White-light emission from this device was uniform in hue over an area of 150×8 mm2, and the module exhibited a luminous flux of 500 lm with a luminous efficiency of 90 lm W−1.
In conclusion, we have developed a phosphor for a violet chip, Cl_MS:Eu2+, based on a newly discovered host crystal with a mixed-ligand system and a layered structure. Cl_MS:Eu2+ exhibited a large Stokes shift, efficiently converting violet light to yellow luminescence, and the luminous efficiency showed good temperature dependence despite the material's layered structure. The use of Cl_MS:Eu2+ in conjunction with violet LED chips allowed us to fabricate glareless pc-LEDs suitable for general illumination with uniform hue, moderate luminance, adequate colour-rendering index and high luminous flux. Furthermore, pc-LEDs prepared with Cl_MS:Eu2+ can be expected to permit the fabrication of light sources with new shapes, such as domes or elongated semicylinders.
Methods
Sample preparation
Single crystals of undoped Cl_MS were grown by the self-flux method, in which SrCl2 acted as both a starting material and a flux. For the formation of a sufficient quantity of liquid flux, SrCl2 was added in excess (7.5 times the stoichiometric amount). The other starting material, SiO2, was also added in excess (1.2 times the stoichiometric amount) because it is not very reactive. SrCl2, SiO2 and a stoichiometric amount of CaCO3, all of 3N or higher purity, were thoroughly mixed and pelletized. The pellets were heated at 1,030 °C for 36 h in air and then cooled to room temperature at a rate of 300 °C h−1. The resulting Cl_MS crystals were collected by washing off the remaining flux with warm water.
We prepared samples of Eu2+-doped Cl_MS by using the method described for Cl_MS, with Eu2O3 or EuCl3 as the Eu source. The Eu2+ fraction per divalent metal ion was 3–50 atom%. The pellets were fired at 1,030 °C for 10 h in a reducing atmosphere of H2/N2 (5/95).
Fabrication of pc-LEDs
Phosphors of different emission colours were mixed at the following weight ratios to provide white emission of specified colour coordinates: Cl_MS:Eu2+/APT:Eu2+=1.8/1.0 for pc-LED sample 1, 100% YAG:Ce3+ for pc-LED sample 2 and (Sr,Ca)AlSiN3:Eu2+/β-SiAlON/APT:Eu2+=0.6/1.1/1.0 for pc-LED sample 3.
Then a phosphor paste was made by dispersion of each of the above phosphor mixtures in translucent silicone resin at a concentration of 0.2–1.3 vol%. Finally, a pc-LED was fabricated by encapsulation of an LED chip on a white substrate with the phosphor paste, which was allowed to harden at 150 °C for 90 min.
Determination of crystal structures
SR-XRD measurements were performed at the Japan Synchrotron Radiation Research Institute, SPring-8, with synchrotron orbit radiation on the BL02B1 and BL02B2 beamlines at a wavelength of ca. 0.35 Å for the single crystals and a wavelength of ca. 0.80 Å for the Eu2+-doped powder samples. The initial atomic positions of Cl_MS were determined directly from the data for the undoped single crystal (see Supplementary Methods).
Optical measurements
The luminescence spectra under continuous excitation and the excitation spectra of the phosphor samples were measured at room temperature with a multichannel optical analyser (PMA C5966-31, Hamamatsu Photonics). Time-resolved luminescence spectra were measured with a pulsed 266-nm laser (CFR 400, Quantel), with an excitation duration of 10 ns and a repetition rate of 10 Hz. IQEs and absorptions were obtained from luminescence spectra with 407-nm laser-diode excitation, using a phosphor sample mounted in an integrated sphere. The detector employed a spectrometer (CAS 140B-152, Instrument Systems). This measurement system had two key features. First, the energy density of the excitation beam with which the sample was irradiated was high. The energy density was as high as actually mounted on an LED chip. Second, the measurement time was short, because a charge-coupled device (CCD) image sensor array was used as a detector. Consequently, we could measure the IQEs without the influence of thermal quenching by the Stokes shift. The integrating sphere had a diameter of 150 mm and three ports with diameters of 25 mm. The sample was placed in the integrating sphere through the bottom port, and excitation light was directed onto the sample from the upper port. Emitted light was directed to the spectrometer through an optical receiver installed in the middle port. We obtained data by gathering the reflections generated by irradiation of the sample with a laser-diode beam (power, 10.2 mW at 407 nm; irradiation time, 10 ms; irradiated area, 1 mm diameter). The detector of the CAS 140B-152 spectrometer was the CCD array, which has 1,024 CCD elements. The wavelength band that could be measured was between 375–785 nm. The reflection spectrum of the BaSO4 powder without absorption was used as a reference for calculation of the IQE and the absorption.
The CAS 140B-152 spectrometer was also used to obtain luminous flux, colour coordinates and colour temperature from a pc-LED operated in an integrated sphere. A two-dimensional colour analyser (CM-1500M, Minolta) was used to obtain the luminance and emission colour distribution on the pc-LEDs.
Additional information
How to cite this article: Daicho, H. et al. A novel phosphor for glareless white light-emitting diodes. Nat. Commun. 3:1132 doi: 10.1038/ncomms2138 (2012).
References
Pimputkar, S., Speck, J. S., DenBaars, S. P. & Nakamura, S. Prospects for LED lighting. Nat. Photon 3, 180–182 (2009).
Taguchi, T. Present status of energy saving technologies and future prospect in white LED lighting. IEEJ Trans. 3, 21–26 (2008).
Bando, K., Sakano, K., Noguchi, Y. & Shimizu, Y. Development of high-bright and pure-white LED lamps. J. Light Vis. Env. 22, 2–5 (1998).
Narukawa, Y. et al. Ultra-high efficiency white light emitting diodes. Jpn J. Appl. Phys. 45, L1084–L1086 (2006).
Narukawa, Y. et al. Successful fabrication of white light emitting diodes by using extremely high external quantum efficiency blue chips. Phys. Stat. Sol. A 205, 1081–1085 (2008).
Kasahara, T. et al. Discomfort glare caused by white LED light sources. J. Light Vis. Env. 30, 95–103 (2006).
Taguchi, T. Present status of white LED lighting technologies in Japan. J. Light Vis. Env. 27, 131–139 (2003).
Hao, Z. et al. White light emitting diode by using α-Ca2P2O7:Eu2+,Mn2+ phosphor. Appl. Phys. Lett. 90, 261113 (2007).
Nishida, T., Ban, T. & Kobayashi, N. High-color-rendering light sources consisting of a 350-nm ultraviolet light-emitting diode and three-basal-color phosphors. Appl. Phys. Lett. 82, 3817–3819 (2003).
Uchida, Y. & Taguchi, T. Lighting theory and luminous characteristics of white light-emitting diodes. Opt. Eng. 44, 124003 (2005).
Takahashi, K. et al. Luminescence properties of blue La1-xCexAl(Si6-zAlz)(N10-zOz) (z~1) oxynitride phosphors and their application in white light-emitting diode. Appl. Phys. Lett. 91, 091923 (2007).
Xie, R. J. et al. Strong green emission from α-SiAlON activated by divalent Ytterbium under blue light irradiation. J. Phys. Chem. B 109, 9490–9494 (2005).
Hirosaki, N et al. Characterization and properties of green-emitting β-SiAlON:Eu2+ powder phosphors for white light-emitting diodes. Appl. Phys. Lett. 86, 211905 (2005).
Fukuda, Y., Ishida, K., Mitsuishi, I. & Nunoue, S. Luminescence properties of Eu2+-doped green-emitting Sr-sialon phosphor and its application to white light-emitting diodes. Appl. Phys. Exp. 2, 012401 (2009).
Park, J. K. et al. Application of Ba2+·Mg2+ co-doped Sr2SiO4:Eu yellow phosphor for white-light-emitting diodes. J. Electrochem. Soc. 152, H121–H123 (2005).
Zeuner, M., Hintz, F. & Schnick, W. Low temperature precursor route for highly efficient spherically shaped LED-phosphors M2Si5N8:Eu2+ (M=Eu, Sr, Ba). Chem. Mater. 21, 336–342 (2009).
Krams, R. M. et al. Status and future of high-power light-emitting diodes for solid-state lighting. J. Disp. Tech. 3, 160–175 (2007).
Taguchi, T. Developing white LED lighting systems and its technological roadmap in Japan. J. Light Vis. Env. 30, 177–182 (2006).
Craford, M. G. High power LEDs for solid state lighting: status, trends and challenges. J. Light Vis. Env. 32, 58–62 (2008).
Fukui, T. et al. Superior illuminant characteristics of color rendering and luminous efficacy in multilayered phosphor conversion white light sources excited by near-ultraviolet light-emitting diodes. Jpn J. Appl. Phys. 48, 112101 (2009).
Notzold, D., Wulff, H. & Herzog, G. Structural and optical properties of the system (Ca,Sr,Eu)5(PO4)3Cl. Phys. Stat. Sol. B 191, 21–30 (1995).
Akella, A. & Keszler, D. A Structure and Eu2+ luminescence of dibarium magnesium orthoborate. Mater. Res. Bull. 30, 105–111 (1995).
Blasse, G., Wanmarker, W. L., Vrugt, J. W. & Bril, A. Fluorescence of Eu2+ activated silicates. Philips Res. Rep. 23, 189–200 (1968).
Kodama, N., Sasaki, N., Yamaga, M. & Masui, Y. Long-lasting phosphorescence of Eu2+ in melilite. J. Lumin. 94-95, 19–22 (2001).
Burrus, H. L., Nicholson, K. P. & Rooksby, H. P. Fluorescence of Eu2+-activated alkaline earth halosilicates. J. Lumin. 3, 467 (1971).
Lin, H., Liu, X. R. & Pun, E. Y. B. Sensitized luminescence and energy transfer in Ce3+ and Eu2+ codoped calcium magnesium chlorosilicate. Opt. Mater. 18, 397–401 (2002).
Zhang, X. & Liu, X. Luminescence properties and energy transfer of Eu2+ doped Ca8Mg(SiO4)4Cl2 phosphors. J. Electrochem. Soc. 139, 622 (1992).
Barkley, M. C., Downs, R. T. & Yang, H. Structure of walstromite, BaCa2Si3O9, and its relationship to CaSiO3-walstromite and wollastonite-II. Am. Mineral. 96, 797–801 (2011).
Park, J. K. et al. White light-emitting diodes of GaN-based Sr2SiO4:Eu and the luminescent properties. Appl. Phys. Lett. 82, 683–685 (2003).
Uheda, K. et al. Luminescence properties of a red phosphor, CaAlSiN3: Eu2+, for white light-emitting diodes. Electrochem. Solid State Lett. 9, H22–H25 (2006).
Kijima, N. et al. New green and red phosphors for white LEDs. J. Light Vis. Env. 32, 202–207 (2008).
Kresse, G. & Furthmüller, J. Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set. Phys. Rev. B 54, 11169–11186 (1996).
Blöchl, P. E. Projector augmented-wave method. Phys. Rev. B 50, 17953–17979 (1994).
Blaha, P., Schwarz, K., Madsen, G. K. H., Kvasnicka, D. & Luitz, J. WIEN2k, An Augmented Plane WaVe Plus Local Orbitals Program for Calculating Crystal Properties (Vienna University of Technology, 2001).
H.Madsen, G. K., Blaha, P., Schwarz, K., Sjöstedt, E. & Nordström, L. Efficient linearization of the augmented plane-wave method. Phys. Rev. B 64, 195134 (2001).
Perdew, J. P., Burke, K. & Ernzerhof, M. Generalized gradient approximation made simple. Phys. Rev. Lett. 77, 3865–3868 (1996).
Yen, M. W., Shionoya, S. & Yamamoto, H. Phosphor Handbook 2nd edn, Ch. 2, 35–47 (CRC press, 2006).
Yoshida, H. et al. Experimental and theoretical investigations for excitation properties of Ba1-xEuxMgAl10O17 . J. Electrochem. Soc. 154, J196–J200 (2007).
Yamamoto, H., Seki, S. & Ishiba, T. The Eu site symmetry in AEu(MoO4)2 (A=Cs, or Rb) generating saturated red luminescence. J. Solid State Chem. 94, 396–403 (1991).
Hwang, K., Hwangbo, S. & Kim, J. Sol-gel synthesis of red-emitting LiEuW2O8 powder as a near-ultraviolet convertible phosphor. Ceram. Int. 35, 2517–2519 (2009).
CIE. Discomfort glare in interior lighting. CIE Tech. Rep. 117–1995 (CIE Publications, (1995)).
Acknowledgements
This research was partially supported by the Ministry of Education, Culture, Sports, Science and Technology Grant-in-Aid for Scientific Research (A), no. 23244074, and the Scientific Research on Priority Areas, no. 20110003. The synchrotron radiation experiments performed at SPring-8 were supported by the Japan Synchrotron Radiation Research Institute. H.H. acknowledges funding from the JSPS FIRST project and MEXT Element Strategy project.
Author information
Authors and Affiliations
Contributions
Y. Shinomiya, T.I., K.E., Y. Sasaki, Y.M. and H.D. synthesized materials and fabricated pc-LEDs. S.A., E.N., M.S. and H.S. carried out SR-XRD measurements and structural analysis. Y. Shinomiya, T.I., K.E., Y. Sasaki, Y.M. and S.M. carried out PL measurements. S.M. and H.H. calculated EFG by DFT. H.D., Y. Shinomiya, S.A., S.M., H.S. and H.H. participated in discussions of the data and the writing of the paper.
Corresponding author
Ethics declarations
Competing interests
The authors declare no competing financial interests.
Supplementary information
Supplementary Information
Supplementary Figures S1-S9, Supplementary Tables S1-S4, Supplementary Methods and Supplementary References (PDF 859 kb)
Supplementary Data 1
Crystallographic data for undoped single crystal of Cl_MS at 100 K (CIF 33 kb)
Supplementary Data 2
Crystallographic data for undoped single crystal of Cl_MS at 300 K (CIF 14 kb)
Rights and permissions
About this article
Cite this article
Daicho, H., Iwasaki, T., Enomoto, K. et al. A novel phosphor for glareless white light-emitting diodes. Nat Commun 3, 1132 (2012). https://doi.org/10.1038/ncomms2138
Received:
Accepted:
Published:
DOI: https://doi.org/10.1038/ncomms2138
This article is cited by
-
Effect of Heat-Treatment on Self-healing and Processing Behavior of Thermally Reversible Polyurethanes
Journal of Polymers and the Environment (2020)
-
Synthesis and photoluminescence properties of the novel Eu3+-activated CaNa(PO3)3 phosphors
Journal of Materials Science: Materials in Electronics (2020)
-
An efficient g-C3N4-based organic hybrid photocatalyst with PEDOT:PSS as a hole-transporting material
Journal of Materials Science: Materials in Electronics (2019)
-
Ultraviolet laser ablation as technique for defect repair of GaN-based light-emitting diodes
Applied Physics A (2018)
-
Effect of sintering temperature on the emission-spectrum-shape-evolution of Sr2SiO4:Eu2+ phosphor
Journal of Materials Science: Materials in Electronics (2018)